An aperture blade is a nickel sheet a few tens of microns thick with a clear bore in the middle, and the rim left around that bore can be as narrow as 20μm. Made one at a time, the bore centre sits within 3μm of the outer diameter, and most shops can hold that. The trouble starts when the blades go up a shaft: three, then five, each off in its own direction, and looking down through the top bore the bottom one has shifted enough to clip the clear aperture. Aperture stack coaxiality is that combined shift. It counts only the part's own contribution, meaning the bore-to-OD offset of each blade plus the tilt built up from thickness tolerance. Pin clearance in the fixture and the machine datum carry their own error, measured and logged separately, never folded into this table.
The scene repeats on the floor. A three-blade set passes the vision gauge at 2.5μm per blade, then stands up in the fixture with 9μm between the top and bottom bore centres, past the 6μm limit. Nobody made a bad blade: the pin sits in the hole with 8μm clearance, all three lean on the same side of it, and the offsets add in one direction. A five-blade set behaves differently. Thickness is called at 50μm and measures 47–53μm, the uneven stack tilts a little, and the error grows with height until the top blade closes on the bore edge. The quietest case of all is flatness at 3μm in spec with an anneal that never went through: stress bleeds out after stacking, and two days on the machine takes coaxiality from 7μm to 12μm. None of this shows on a single-blade report. The stack has to be stood up and checked in transmission.
Parameter Window
• Bore centre to OD within 3μm per blade, bore tolerance ±3μm, narrowest rim 20μm
• Stack coaxiality by count: 3μm for one blade, 6μm for three, 10μm for five, in-house measured ranges rather than a standard
• Blade thickness 40–80μm at ±2μm, five blades stacking to 200–400μm
• Pin-to-hole clearance held at 5μm or less, booked as fixture error and kept off the stack table
• Bore wall roughness 0.01μm or better, checked blade by blade; stacking does not average scatter away
• Flatness 3μm per blade, remeasured after 180°C for 1h, then released to pairing
Manufacturing Process (8 Steps)
1. Layout — bores and outlines come off one drawing, the outer diameter sets a single datum, and nobody re-derives coordinates downstream.
2. Pre-treatment — clean and make the substrate conductive so plating starts evenly, or the rim thickens before the centre fills.
3. Resist and LDI — 8μm/8μm resolution with ±5μm double-sided registration, bore and OD exposed in one pass.
4. Development — open the bore 2–4μm over size for compensation, no residue at the mouth, no undercut at the rim root.
5. Plating — 1–4 A/dm² up to 40–80μm, hardness landing between 450 and 550HV.
6. Release and anneal — peel from a low-stress corner, anneal at 180°C for 1h, let the internal stress go before talking accuracy.
7. Single-blade inspection — vision gauge reads bore centre against OD, rejects are pulled, good blades binned by offset direction.
8. Pairing and stacking — pair plus against minus bins, stand the stack in the fixture, read top and bottom bore centres in transmission, log the result.
Core Advantages
1. Directional pairing cancels about half the offset; a three-blade set often comes down from 9μm to roughly 5μm without forcing anything.
2. The stack table and the fixture error table stay apart, so aperture stack coaxiality trouble is traced to a blade or to a pin, not to both at once.
3. The 3μm single-blade limit is a gate: a blade that misses it never reaches pairing, which keeps a whole stack from being reworked.
4. Thickness at ±2μm limits stack tilt, which is what keeps five-blade drift inside the 10μm line.
5. Annealing happens before pairing, so stress is gone and the stack does not drift again after a few days on the machine.
6. Each stack keeps its pairing map and end readings, so a customer remeasurement can be walked back blade by blade.
Typical Applications
1. Variable iris assemblies in lenses, three to five blades stacked, bore opening and closing by stop.
2. Mode-limiting apertures in lasers, blades in series to cut stray light, where coaxiality sets beam quality.
3. Entrance slit stacks in spectrometers, slit width built from blade count and thickness.
4. Beam-limiting bores in electron guns, where an off-centre stack smears the spot.
5. Stray-light suppression rings in camera modules, bore and ring on one axis to block oblique rays.
6. Beam baffle stacks in coating chambers, where blade offset defines the uniform deposition band.
Design and Selection Notes
1. Fix the blade count, then the tolerance. Quote 10μm for five blades and 6μm for three, and never promise a stack on the strength of a 3μm single blade.
2. Fewer blades is not automatically easier. Push one blade past 150μm and bore taper and burr hurt transmission more than stack offset does.
3. Pair by direction, not by number alone. Two blades off 4μm in opposite directions stack to about 1μm.
4. Calibrate the fixture separately. A 5μm pin clearance can grow to 9μm across five blades, and that is not the part's account.
5. If a five-blade stack passes 10μm, send it back to pairing; do not clamp it straight in the fixture, because a pinched blade springs back.
6. Read flatness and thickness together. One blade warped 3μm becomes a dozen microns of tilt across five.
7. Sample by stack, not by blade. Two stacks out of ten stood up in transmission reveal drift that twenty loose blades will hide.
Take aperture stack coaxiality apart and it comes down to two moves: pull each bore to within 3μm of its OD, then pair the offsets so their directions oppose. The first is exposure and development, the second is binning and records. Loosen either and five blades drift a dozen microns while every single-blade report stays green. On the floor each stack is stood up under a 200× vision gauge, read from the top bore down to the bottom, and anything past 10μm is stripped and re-paired rather than clamped or reamed. Time is the other thing people miss: a blade with an incomplete anneal will drift another 3–5μm after two days in the machine, so remeasuring flatness after anneal is not optional. With aperture blades, a good single-blade number is easy. Twenty stacks from one lot, month after month, all inside the bin table, is the real work. When ordering, state blade count, thickness tolerance, pairing direction and who owns the fixture error; that settles more arguments than any post-mortem.