Kunshan Electroformed Mesh Processing: Mesh Count Deviation and Screen Tension

kunshan electroformed mesh processing

Kunshan electroformed mesh processing describes a screen delivered to customers in the Kunshan area: the aperture layout for a given mesh count is written into a resist pattern, nickel is electroformed into a mesh, and the screen is framed, tensioned and checked zone by zone. Mesh count is not a label stuck on the frame; it is derived from aperture size and opening spacing. When a customer asks for 300 mesh, the line checks aperture tolerance ±3 μm and opening spacing ≥50 μm against the drawing. Drawings common among Kunshan and nearby customers put roundness ±0.002 mm in the screen zone. The final inspection post calibrates the image instrument against a reference piece every day so the reading counts.

Most failures show up on the mesh surface. One batch was ordered as 200 mesh and the image instrument counted only 197; development undercut had enlarged the apertures by 3 μm and the derived count dropped a step. Another screen looked flat but paste piled up on one side and thinned on the other in printing; the tension gauge read from 16 N to 24 N because AB adhesive frame cure time had been shortened. A third customer held a mesh to the light and found elongated apertures beyond the ±0.002 mm roundness band, so the inspection machine rejected it. Whether that screen is reworked or scrapped depends on whether a fresh lamination can recover the ovality. Bath chemistry was never at fault. Kunshan electroformed mesh processing has to catch the pattern stage and the tension stage.

Parameter Window

• Mesh count is derived from measured aperture and opening spacing; deviation is given as a ±1–2 mesh range, not an absolute accuracy class.

• Micro-aperture tolerance ±3 μm, minimum opening 25 μm and opening spacing ≥50 μm are sampled zone by zone.

• Screen roundness ±0.002 mm; the image instrument samples the length-to-width ratio of apertures, and an oval beyond the band is stripped.

• Nickel layer 30–150 μm in bands, current density 1–4 A/dm² in steps, so the aperture walls stay free of nodules.

• Nickel alloy hardness 450–550 HV and low-temperature annealing relieve stress; an uneven screen sends the operator to the annealing curve.

• Tension 10–55 N with ±1 N internal control; the AB adhesive frame cures at 23 ± 2 °C before the tension reading is taken.

Manufacturing Process (8 Steps)

1. Drawing review — check the mesh count derivation, ±3 μm aperture tolerance and ±0.002 mm roundness, then set the window by aperture density.

2. Substrate prep — 610 × 660 mm carrier plate, degrease, clean and dry; no visible dust in the clean area before lamination.

3. Lamination and exposure — hot-roll the dry film flat and write the aperture array at LDI resolution 8 μm/8 μm.

4. Development — temperature and spray follow the band, fine apertures get a few extra seconds, and undercut goes into the count compensation.

5. Pattern re-measurement — image instrument samples aperture and roundness, flash tester samples opening spacing, and readings stay on the traveller.

6. Electroforming — 1–4 A/dm² in steps, nickel grows inside the windows to 30–150 μm.

7. Resist strip and peeling — strip the film and lift the nickel mesh off in one piece, with no residual resist and no torn edge.

8. Final tension check — AB adhesive frame pulled to 10–55 N, full-area scan, photo filed, and only then packed.

Core Advantages

1. Mesh count can be audited — every derivation keeps the measured aperture value and the deviation is reported as a range that a customer can recheck.

2. Apertures keep their shape — development undercut goes into compensation and roundness ±0.002 mm is held at the pattern stage.

3. Tension is read by zone — 10–55 N is logged point by point at ±1 N, and a screen mixing 16 N with 24 N never leaves the shop.

4. No new frame on a changeover — the AB adhesive frame goes back on the bench; a new mesh count only needs fresh film and exposure.

5. Data can be traced back — film lot, development temperature, exposure order and tension readings share one page of the record.

6. Rework stays upstream — a deformed aperture or excess undercut found at the pattern stage means stripping and redoing, saving plating hours.

Typical Applications

1. Screen-printing meshes, where paste throughput is held by ±3 μm aperture tolerance.

2. Printing mesh foils for semiconductors, minimum aperture 25 μm, with development undercut compensated separately.

3. Battery paste filter screens, opening spacing ≥50 μm and roundness ±0.002 mm to control flow resistance.

4. Micro-aperture nickel foils at ±3 μm aperture tolerance, sampled zone by zone so no step drops out.

5. Aperture plates and encoder screens with fine ribs mixed into the array, scanned zone by zone for broken ribs.

6. Prototypes and short runs, where only the exposure card changes and the frame and substrate carry on.

Design and Selection Notes

1. Mesh count is not the higher the better — below 25 μm openings paste tends to clog, so choose the band by real throughput.

2. Derive count from measured apertures; do not reconcile against a nominal count, and discuss deviation as a ±1–2 mesh range.

3. Development temperature belongs on the process card; undercut drift beyond 2 °C sends the job back to the inspection machine.

4. Judge roundness and aperture apart: ±0.002 mm is shape and ±3 μm is size, and mixing them misreads the result.

5. Keep tension in the middle of 10–55 N; past 55 N the adhesive creeps and the mesh surface goes wavy.

6. A new film lot means a fresh compensation scan, not the previous undercut coefficient.

7. Kunshan electroformed mesh processing gives ranges from measured values and promises no absolute accuracy; the window locks only after the drawing is confirmed.

Take Kunshan electroformed mesh processing apart and the two issues separate cleanly: count deviation comes from development undercut, screen tension from cure and framing, and they do not belong on one reject sheet. On the bench, a screen passes when the image instrument reads aperture and roundness, the flash tester reads opening spacing and the tension gauge is logged by zone; any reading on the limit sends it back for a fresh lamination. Nickel thickness, hardness and tension go onto the traveller so a customer re-measuring against the same criteria has nothing to argue about. If undercut drifts past the compensation matched to 2 °C, go back to the development stage and re-measure the apertures instead of overturning the call at final inspection. Kunshan electroformed mesh processing reports deviation as a range derived from measured apertures and grouped by lot, with no absolute accuracy class and no universal mesh grade. A full-area photo is filed before dispatch so a customer can call the record up when incoming material is re-measured; the delivery and communication basis for customers in the Kunshan area follows that card, and retained data keeps any dispute grounded.