An electroformed mask is a thin nickel-alloy sheet with openings cut in it, laid on the substrate during evaporation, and the openings decide what gets coated. Magnets hold it down, and how flat that face sits once it is pulled in decides how deep a channel the vapour finds on its way in at an angle. Electroformed mask magnetic-clamp flatness means flatness in the clamped state and the shadow deviation worked out from the gap. The number taken on a granite table, with nothing pulling on the sheet, is a different measurement.
An evaporation plant in Ningbo returned one sheet that read 8μm on granite and passed, then lifted 30μm at the corners on the magnetic chuck and coated 12% thin at the edge. A second one was pushed up in the middle by a 3μm residue spot on the chuck; the magnets bowed the mask into a dome and the whole sheet was lost. A third had magnets spaced unevenly, held in the centre and floated at the rim, a 15μm gap difference that changed the shadow width and fuzzed the pattern edge. Three returns, three times the same root cause: the part was measured under a different clamp than the one it runs in.
Parameter Window
• Mask thickness 20–100μm; thinner clamps better, but under 20μm the sheet buckles and the gap doubles at each wave
• Flatness in the clamped state 10μm or better over 100×100mm, sampled at the corners as well as the centre
• Contact gap between mask and substrate 5–12μm; past 15μm the shadow starts eating line width
• Incidence 30–45°, shadow estimated as gap times tan of the angle, so 10μm at 45° gives about 10μm
• Rib 20μm and opening 30–60μm; once shadow takes a third of the rib, the magnet layout is the problem
• Magnet pitch 25–50mm with 3–10 kPa of clamping pressure, laid out to match the chuck hole pattern
Manufacturing Process (8 Steps)
1. Layout — arrange the openings on the array, ribs from 20μm up, and keep a 3–5mm magnetic border; a narrow border will not hold.
2. Pre-treatment — clean the substrate and make it conductive, holding the starting surface inside 2μm.
3. Resist and LDI — 8μm/8μm resolution with ±5μm double-sided registration, openings and ribs in a single image, no stitching.
4. Development — open the features 2–4μm over for line width compensation and strip residue, or nodules grow on the edge.
5. Plating — 1–4 A/dm² of nickel-cobalt at 50±2°C, thickness set between 20 and 100μm by mask size.
6. Anneal — 180–200°C for 1h to relax plating stress so the sheet lies flat on its own.
7. Release — peel slowly from a corner, always the same direction, and leave no crease across the face.
8. Remeasure — clamp on the magnetic chuck and scan a 5×5 grid with a laser gauge, reading flatness as clamped.
Core Advantages
1. Electroformed mask magnetic-clamp flatness is quoted as clamped. A sheet at 5μm free and 20μm clamped is not a 5μm sheet.
2. Shadow deviation is worked out before the hardware changes: 10μm gap at 45° means 10μm of shadow, so the magnet bill comes first.
3. Magnet pitch and pressure follow the chuck pattern, so clamping consistency comes from layout rather than operator feel.
4. Proper annealing means a sheet taken off and put back reads the same band, instead of curling a little more each week.
5. Remeasurement uses the customer's clamp, which keeps the two sites within 3μm of each other and halves the arguing.
6. Opening, rib and flatness are measured on three separate books, so a failure points at one cause instead of the whole sheet.
Typical Applications
1. Fine metal masks for OLED evaporation, openings from 30μm and ribs at 20μm, where any shadow costs colour purity.
2. Mask sheets on optical coating domes, at steep incidence and sensitive to a 5μm gap change.
3. Sensor window coating masks, where the seal face has to close all the way round.
4. Backside coating masks for semiconductor work, 30μm sheet, wrinkling at the least uneven pull and doubling shadow at the crease.
5. Decorative coating masks with large area and many openings, held down by an even magnet field.
6. Wafer-level packaging masks, where the gap lands directly in line width, with no room on a 20μm rib.
Design and Selection Notes
1. Clamp the way the customer clamps. An 8μm reading from granite and vacuum does not carry over to a magnetic chuck.
2. Thinner is not better. Below 20μm the sheet loses stiffness, buckles under the magnets and throws a wider shadow.
3. Look at the chuck before the mask. With no magnet in the middle, the middle floats, and extra thickness will not save it.
4. If the gap passes 15μm, go back to the remeasurement bench and check electroformed mask magnetic-clamp flatness and magnet strength first, then talk about incidence.
5. Past 45°, every extra 5μm of gap adds 5μm of shadow, so a 20μm line is run at a 10μm gap.
6. Scan a 5×5 grid with all four corners, not three rows across the middle; the corners are what decide the call.
7. Store the sheet flat. Left standing against a wall overnight, it comes back 10μm worse in the morning.
Once electroformed mask magnetic-clamp flatness is treated as a clamped quantity, the argument shrinks. The same sheet reads 6μm free and 14μm under magnets; the 8μm between them is the bow that the field flattens and then lets spring back. On the floor the bench carries the customer's own chuck type, magnets on a 30mm pitch, and the laser gauge walks 25 points; any corner over 10μm gets flagged and the chuck is checked for residue or a magnet fitted backwards. A sheet past a 15μm gap is not ground down first. Somebody works out what fraction of the rib the shadow takes, and at a third, polishing the surface will not bring the pattern edge back. One sample at 8μm clamped is not the hard part. Twenty sheets, across three chucks, all still inside 10μm, is.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292
Email:yw9@zldsmt.com
Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋