The sidewall angle of an electroformed mask opening is the angle between the hole wall and the mask face. It is a cross-section figure and a separate account from planar linewidth. Quality takes readings on a metallographic section or an optical profiler, five points in all (centre plus four corners) and reports the mean and the range. On a 20–50 μm mask the target sits at 88–90°; one point off by 1° goes to re-measurement, anything past 2° is scrapped outright — replating can rescue planar size but never the direction the wall leans.
An evaporation source has a spread angle, and a 0.1–0.5 mm gap stays between mask and substrate. Give the wall just 1° of taper and the projected boundary shifts 2–9 μm: pattern edges go soft and lines at tile joints refuse to line up. A trumpet mouth is worse — wide at the top, narrow at the bottom, boundary errors point opposite ways on the two sides of one sheet, every planar dimension passes, and the whole evaporation run still fails on boundary. One batch passes on one machine and fails on the next, the difference sitting in gap and angle rather than the sheet. The trail ends at the section: the sidewall angle of an electroformed mask opening and linewidth compensation govern different things.
Parameter Window
• Sidewall target 88–90°, taper ≤2°; a point 1° off goes to re-check, past 2° is scrap
• Hole wall roughness ≤0.01 μm, to cut re-deposit and bounce-back on the wall
• Opening size ±3 μm, position ±7 μm, accepted on the same sheet as the section angle
• At 0.1–0.5 mm gap each degree of taper shifts the boundary shadow 2–9 μm; budget it against the source spread
• LDI resolution 8 μm/8 μm, double-side alignment ±5 μm — the resist profile is upstream of the angle
• Five sampling points (centre plus four corners), angle range ≤1.2°, sheet kept for 3-month re-check
Manufacturing Process (8 Steps)
1. Opening and angle design — work projected size back from source spread and evaporation gap; put the target sidewall angle on the drawing.
2. Substrate prep and coating — degrease, coat photoresist, laminate free of bubbles; the resist profile sets the later section.
3. LDI exposure — 8 μm/8 μm resolution, double-side alignment ±5 μm, dose calibrated per resist thickness.
4. Development — bath at 23±2°C, time window narrowed to ±5 s, no roll-back at the hole mouth.
5. Electroforming — current density 1–4 A/dm², start slow to hold stress down so taper does not pile up during growth.
6. Stripping — peel off the mandrel with even force; once a tear starts, the hole-mouth angle changes on the spot.
7. Section and size inspection — profiler or section for the five angle points, vision system for openings, flash gauge across the panel.
8. Verdict and re-check — within 1° records as a concession, past 2° is scrap; keep samples and re-read stress spring-back at 3 months.
Core Advantages
1. Angle and planar size reported apart — ±3 μm and 88–90° each hold their own line on the drawing and neither stands in for the other.
2. Shadow can be estimated up front — plug gap and taper in and the boundary shift is settled at the sampling stage.
3. Sampling with a method — five points, centre and corners, range in the report; one good point never carries a whole sheet.
4. Scrap line in the open — 1° concession, 2° scrap, no bargaining at the line.
5. Ageing tracked — one round at shipping, one at 3 months, so nickel stress spring-back shows up early.
6. Checked together with framing — angle passes first, then 10–55 N tension; deformation risk counted separately.
Typical Applications
• Metal masks for OLED evaporation, where soft edges eat yield directly
• Optical filter shutters, narrow band patterns fussy about edge sharpness
• Sensor array masks, where boundary error accumulates along the array
• PV grid-line shutters, whose tile joints live on the angle
• Medical device directional evaporation masks, mostly 30 μm class small openings
• Section data from sampling runs, to confirm the projected boundary is good enough
Design and Selection Notes
1. Mark the angle on its own. Planar width and wall direction are two accounts; linewidth compensation will not carry it.
2. Fix the gap first. Clamped at 0.1 mm or floating at 0.5 mm, the same 1° taper differs fivefold in shadow.
3. Closer to 90° is not automatically better — too steep piles stripping stress at the mouth, and service life pays for the angle.
4. If the angle reading drifts past 1° on two sheets in a row, go back and re-check exposure dose and development time instead of only touching the bath.
5. Put the scrap threshold in the acceptance clause; concessions get written down, verbal ones cannot be untangled later.
6. On dispute the metallographic section rules — the profiler is fast and non-destructive, but arbitration still looks at the section.
7. On old sheets re-read angle before size; stress relief usually shows on the wall first.
At the inspection bench the sidewall angle of an electroformed mask opening is one profile trace plus five numbers. The inspector plots: centre 89.2°, corner 87.9°, range 1.3°, so per internal rules it goes to re-check before any concession; past 2° replating is useless, the section stays crooked and the sheet is scrap. The evaporation side wants its account early: gap 0.5 mm, taper 1°, boundary moves 8.7 μm, and whether that fits should be settled at the sampling stage. Once the sidewall angle of an electroformed mask opening is managed as its own figure, boundary error becomes something with a budget; it and linewidth compensation, one governs planar width and one the way the wall leans, written apart on the drawing and measured apart on the line. If angle readings drift past 1° on two sheets after clamping, go back to exposure and development for re-check rather than plating on. For orders with evaporation boundary requirements, fix the target angle, sampling points, concession line and 3-month re-check into the acceptance sheet together. What ships is the sheet whose five points all land in 88–90°, with boundary error that can be budgeted.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292