Welcome: Shenzhen Zhuolida Electronics Co.TD
Language: Chinese ∷  English
Your location: Home > News > Company new

Company new

XRF Thickness Comparison on Electroformed Parts: A Submission Protocol for Non-Destructive Gauging

XRF thickness comparison on electroformed parts

XRF gauging fires a beam at the part, excites the characteristic fluorescence of the coating elements, and watches the count climb with thickness until it saturates; the instrument converts that into microns off a stored curve. Nothing is touched, nothing is sectioned, and the part ships straight after the reading. The trouble sits in the same place as the convenience: the number is an average over a small patch, and whether it means anything depends entirely on the baseline written into the submission. XRF thickness comparison on electroformed parts means putting that number next to a stated reference, either a coating standard shipped with the lot, a bare substrate of the same alloy, or a retained coupon cut for metallography. When QA holds up a disc and asks whether 48μm passes, the answer is not on the screen. It is in the baseline field of the report.

Three things happen on the floor, over and over. One disc reads 51μm at the rim and 46μm at the centre, the customer takes the centre figure and calls the lot thin, when a 1mm spot had straddled the step fillet and measured a projection on the slope. Another lot goes out against a nickel standard that had not been recertified in two years; the surface had dulled with oxide and every reading ran 0.8μm high until a cross-section pulled it back. The third is the saddest: parts measured straight out of the bath with a film of water still on them read 2–3μm high, and settle back after two hours in a 23±2°C room. None of the three is a broken instrument. Each is a protocol nobody pinned down.

Parameter Window

• Coating coverage 20–120μm; below 15μm the fluorescence is too sensitive to surface contamination and the reading is indicative only

• Baseline stated in the report, one of three: matched coating standard, bare substrate of the same alloy, retained metallographic coupon at a 5-point average

• Spot from 0.3mm up, points at least 2mm off any edge; ribs under 0.15mm wide get a 0.1mm spot or the substrate signal leaks in

• Dwell 20–30s per point, 5 points averaged per part; spread above 3μm between first and last point triggers 4 more points and a 9-point average

• Standard recertified by a third party every 12 months, checked against a reference coupon at every shift start, drift past 0.5μm stops the line for recalibration

• Verdict rule: within ±5% or ±3μm of the baseline, whichever is larger, passes; anything outside is remeasured elsewhere before repair or scrap is decided

Manufacturing Process (8 Steps)

1. Job registration — log alloy, nominal coating thickness, substrate and surface condition, file the traveller with the part, and do not schedule a job with fields missing.

2. Surface check — naked eye plus 10× magnification, clear oil, water film and fingerprints with anhydrous ethanol, leave no lint behind.

3. Baseline selection — align the standard with the part on coating element and substrate alloy; where they do not align, switch to a bare substrate, never mix the two.

4. Warm-up and calibration — 15min warm-up, reference coupon verified, filter matched to the coating element, and the reading has to land on the certificate value before anything is measured.

5. Point layout — mark the working face from the drawing, five points in a cross or quincunx, clear of fillets, steps, clamp marks and laser marking.

6. Point-by-point measurement — 0.3mm spot, 20s dwell, no more than 3 exposures on one point so local heating does not bias the count.

7. Verdict and remeasure — read the spread before the mean; a part with a passing mean and a spread above 8μm is flagged, and 4 points are added elsewhere.

8. Report and retention — the report carries baseline, spot, point count, mean and spread, and one part per lot is sealed as a coupon for the customer's remeasurement.

Core Advantages

1. With the baseline on the first line of the report, XRF thickness comparison on electroformed parts is traceable, and a failed remeasurement can be walked back to its reference.

2. A 0.3mm spot averaged over 5 points flattens local variation, which represents a whole disc far better than any single reading.

3. No contact and no sectioning, so a 20–120μm finished part goes to the next operation with no destructive coupon sacrificed.

4. The shift-start coupon check keeps drift inside 0.5μm, so a reading cannot wander off across an entire lot unnoticed.

5. The verdict rule is settled at quotation, with the repair threshold and the scrap threshold agreed before shipment rather than argued after it.

6. Cross-checking against metallography settles doubt: cut one part, and accept the report only when the two routes land within ±3μm.

Typical Applications

• Nickel coating sampling on electroformed encoder discs, 20–120μm part by part, judged on within-part spread rather than the mean.

• Thin coating checks on aperture blades, 15–40μm parts read with a 0.1mm spot held on the rib to avoid substrate dilution.

• Incoming inspection of electroformed stencil sheets, 3 sheets sampled at 5 points each and compared line by line with the supplier report.

• Nickel plating measured over etched parts, where a stainless substrate forces a bare-substrate baseline instead of the nickel standard.

• Before-and-after comparison on reworked parts, with the same point positions after a 10–20μm touch-up so the numbers stay comparable.

• Complaint reproduction, where both sides measure once and align on baseline first, point count second, since most disputes sit in those two fields.

Design and Selection Notes

1. Put the baseline on the drawing or the purchase order before submission. A bare callout of 50μm coating hands the verdict to whatever default the instrument carries.

2. More points is not the same as more accuracy. Nine points across a 30mm disc cover the thickness variation so fully that the mean goes blunt.

3. A substrate change means a new baseline. Nickel over nickel and nickel over stainless sit behind completely different absorption corrections for the same reading.

4. Keep large spots away from thin coatings. Below 15μm, a 1mm spot lets substrate fluorescence past half the signal and drags the reading 2–4μm low.

5. If the reference coupon drifts past 0.5μm, stop measuring and recalibrate in house; do not apply an offset to the readings and call it correction.

6. Agree the remeasurement protocol with the customer on four items, spot, point count, baseline and verdict threshold. That settles more than comparing instrument prices.

7. Report the spread. A part with a passing mean and an 8μm spread still misbehaves in the machine, and the customer will ask about it sooner or later.

What makes XRF thickness comparison on electroformed parts hold up is not the price of the gauge but the few lines written before submission: which baseline, what spot, how many points, how much drift counts as out. The floor routine is plain. The part enters the inspection room, the surface is checked, the certificate date on the standard is read, and the spread goes into the report alongside the mean. One lot of 60μm discs averaged 59μm and looked fine, with a 9μm spread; on the encoder the signal amplitude wandered high and low, and the cause was a thin band of coating around the rim. A mean can lie on paper. A spread rarely does. The number belongs to the instrument, the protocol belongs to the people holding it.

CATEGORIES

CONTACT US

Contact:赖先生

Phone:+86 18938693450

Tel:0755-2708-8292

Email:yw9@zldsmt.com

Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋

Scan the qr codeclose
the qr code