Reflectance drift of electroformed encoder discs is the curve along which the reflectance gap between bright grating lines and dark gaps widens or narrows once a disc has left the plant. The reading taken at shipping is the steady-state figure, and it governs whether a new disc passes; this basis admits only the time series in service — same spot, same 660 nm source, same incidence angle, re-tested quarterly, judged on slope. The metrology room holds 23±2°C, the spot is locked at 0.5 mm, and every disc gets an R0 and C0 pair on file when it is logged.
Three troubles eat the most time on the floor. A servo motor runs 4000 h and the encoder A-phase amplitude falls from 1.2 Vpp to 0.7 Vpp, counts start dropping, and the disc face is not scratched at all — a film of oil mist has settled on the line edges. Another: two new discs from one batch differ by 8 points of contrast, and on one read head one runs steady while the other jumps. A third: a customer measures at 850 nm while our report was written at 660 nm, the numbers refuse to match, and the rework goes the wrong way. All three accounts get settled by re-testing over time.
Parameter Window
• Initial reflectance 55–70% at 660 nm, normal incidence, φ0.5 mm spot, room at 23±2°C
• Grating contrast C=(R bright−R dark)/(R bright+R dark) ≥60%; new discs usually land at 68–74%
• Drift verdict: ΔR ≤5% of the initial value, or ≤3 points a year, whichever bites first
• Cadence: one round every 500 h in continuous running, every 3 months in stores, at least 3 points
• Track width 50 μm ±0.5 μm, line sidewall roughness Ra ≤0.01 μm
• Disc thickness 0.10–0.30 mm, nickel-cobalt coating HV450–550, thickness spread ≤5 μm
Manufacturing Process (8 Steps)
1. Substrate preparation — glass cleaned and made conductive, stray particles held below 25 μm.
2. Electroforming — nickel sulfamate with cobalt, 1–4 A/dm², hardness landing in HV450–550.
3. Grating forming — LDI at 8 μm/8 μm, double-side alignment ±5 μm, track held to 50 μm ±0.5 μm.
4. Thickness levelling — ground to 0.10–0.30 mm, spread within one disc ≤5 μm so it does not bow when clamped.
5. Stripping — the electroform is peeled off the mandrel; the peeled face is the working face and gets no second polish.
6. Cleaning and passivation — ultrasonic plus deionised water, film 5–10 nm; a thicker film eats reflectance.
7. First calibration — 660 nm source at fixed incidence, R0 and C0 issued and filed against the serial number.
8. Time-series re-test — same spot again at the 500 h or 3-month point; a slope out of band sends the lot back through the process.
Core Advantages
1. Slope instead of single points. The absolute value leans too hard on cleanliness; the slope does not lie.
2. Optical geometry locked: source, incidence and spot written on the method card, so a different operator still matches.
3. Fixed spots, five in the line zone and five in the gap zone, following the file rather than a convenient choice.
4. One reference disc per batch never enters production; it ages alongside as a live sample.
5. Reports carry the serial number, so disc, read head and data string together without digging through chat logs.
6. Kinks can be attributed: a sudden bend means contamination or passivation film, a gentle ramp means the material.
Typical Applications
• Incremental encoder discs for servo motors
• Absolute discs for robot joints
• Indexing discs for CNC rotary tables
• Speed feedback discs for medical pumps
• Fine-track discs for photoelectric theodolites
• Spare discs that sat in stores over a year
Design and Selection Notes
1. Match the wavelength first. If the machine runs 850 nm, do not accept a 660 nm figure; the silicon cell responds very differently.
2. Contrast outranks absolute reflectance; once C falls under 45% the signal amplitude has usually lost a fifth.
3. Wiping more is not wiping better — ethanol residue lifts the initial figure and fogs the disc faster later.
4. If ΔR passes 5%, go back to cleaning and coating thickness before scrapping the disc.
5. Test stock too; a disc stored 12 months often walks 3 points.
6. Put the room temperature on the report — a 10°C swing eats 1 μm of track margin, and thermal growth has to come out of the reading.
7. Only batches at Cpk ≥1.33 are worth a slope; where the scatter is already wide, a regression line means nothing.
In the metrology room this re-test is one lamp, one fixed angle and a form filled in by quarter. The inspector sets the disc on the stage, throws the 660 nm source onto the line zone, records R0 and C0, and from then on fires at the same spot every 500 h or every quarter, joining two points to read the slope. One batch ran a full 4000 h with ΔR at 1.8 points, C easing from 72% to 68%, and was released to keep running. Another lost 6 points in 1500 h; opened up, the passivation film was thick and oil mist had settled on it, and after cleaning it came back to 3.2 points, inside the ≤5% band, so it was washed rather than scrapped. The split against the shipping reading is clean: the steady figure decides whether a new disc passes, the time series decides how long it lasts. If the slope passes 3 points a year at two consecutive points, go back to coating hardness and the cleaning step before blaming the read head. Higher reflectance is not better either: discs pushed above R0 75% tend to carry a thin passivation film and fall faster after half a year. For servo or rotary-table orders that run for years, write the wavelength, incidence, sampling period, ΔR limit and the three re-test points into the technical agreement, and re-test on the same method card after any head change. What ships is a time series with slope ≤3 points a year and C still ≥60%.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292
Email:yw9@zldsmt.com
Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋