Edge slitting quality of precision nickel mesh comes down to two things: how much burr is left on the cut edge, and how far the cut blank sits from the drawing. This is not the micro-punching done on aperture blades — that argument is about cutting-edge profile, while this one is coil stock being cut to size, half a metre wide, with thousands of apertures along the edge to answer for. The verdict keeps two books apart: the burr book records height and root width, the dimensional book records width, length and diagonal. Merge them into one sheet and nobody can tell whether to move the knife or change the drawing.
Three losses have been paid for on the floor. A winder takes up 300 m and the edge burr combs thin scratches into the next layer, showing up as a row of marks when unrolled. Second, an edge curls inward 0.2 mm after slitting and lifts all round when bonded to the frame; adhesive pressure will not flatten it. The third costs most: width runs 0.12 mm over and the whole coil will not enter the customer's tensioning fixture, so a hundred-odd metres gets downgraded. Somebody also judges burr under a 10× loupe and calls it good while the customer's confocal reads 9 μm, and the two sides argue for a fortnight. Different gauges, no common number.
Parameter Window
• Burr height ≤5 μm and no more than 10% of material thickness, both at once
• Width tolerance ±0.05 mm up to 50 mm, ±0.10 mm from 50 to 200 mm, ±0.15 mm above 200 mm
• Cut length ±0.20 mm, diagonal difference ≤0.15 mm, edge straightness ≤0.10 mm per 500 mm
• Cut-edge collapse ≤8 μm, edge roughness Ra ≤0.4 μm, no roll-over and no tear band
• Material 20–100 μm, aperture tolerance ±3 μm, open area within ±3% of drawing
• Apertures within 3 mm of the edge stretched ≤8 μm, edge curl ≤0.10 mm
Manufacturing Process (8 Steps)
1. Incoming check — thickness 20–100 μm, aperture ±3 μm and open area measured; edge scrap pulled first.
2. Stress relief — low-temperature anneal, coil rested flat for 24 h before the machine, so it does not spring back after cutting.
3. Film both sides — 30–50 μm protective film top and bottom so swarf cannot chip the apertures during the cut.
4. Vision alignment — CCD tracks the edge, first article cut with 5 mm spare, edge distance set by drawing.
5. Precision cutting — knife clearance at 8–12% of thickness, 2–3 μm for 20 μm stock, tension held constant.
6. Electrolytic deburring — a light edge polish takes off the 3–5 μm tips without rounding the apertures.
7. Clean and dry — deionised rinse, swarf flushed out so it cannot press marks into the mesh later.
8. Inspection — vision system for width, confocal for burr, snap gauge for the diagonal.
Core Advantages
1. Film before the knife; aperture chipping drops sharply and the cut edge comes out much cleaner.
2. Clearance follows thickness — 20 μm and 100 μm run two different parameter sets, not one compromise.
3. Burr judged on two counts, height and root width, because height alone misses thin long fins.
4. Fixed sampling: five points at both ends and the middle, maximum decides, no picking the pretty spot.
5. The dimensional book stands alone; width, length and diagonal are logged apart, so an overrun traces to knife position or feed.
6. Curl gets its own limit, 0.10 mm, or the sheet will lift at all four sides in a tensioning fixture.
Typical Applications
• Current-collector mesh blanks for lithium cells
• Cut-to-length precision filter mesh
• EMI shielding mesh blanks
• Speaker dust mesh punched to shape
• Support mesh for fuel-cell diffusion layers
• Sensor dust mesh in small lots
Design and Selection Notes
1. Band the tolerance by width; holding ±0.05 mm above 200 mm sends cost up sharply.
2. Write the burr limit as an absolute plus a percentage — at 30 μm stock, 5 μm is already 17%, so the tighter one rules.
3. A sharper knife is not automatically better; too fine an edge drags a tear band through thin stock and the burr gets worse.
4. If burr passes 5 μm on three coils running, go back to clearance and film tension rather than winding the speed down.
5. Check straightness and curl together; straight but curled stock still lifts once it is in the fixture.
6. Sample to GB/T 2828.1 general level II at AQL 0.65, with the burr item tightened one step.
7. Measure within 48 h of slitting; nickel mesh springs back slowly and a week later the width reads 0.03 mm loose.
On the inspection bench, edge slitting quality of precision nickel mesh is two instruments and a caliper. The first article comes off the machine and the inspector reads width on the vision system: 50.02 mm against a 50 mm nominal, inside ±0.05 mm. The edge strip then goes under the confocal and five points are taken along 100 mm; the tallest burr is 4.2 μm on 40 μm stock, which is 10.5%, so that coil goes to rework — not scrap, one light electrolytic pass still saves it. Another coil measures 50.11 mm, 0.06 mm over, and drops to a narrower grade. Keeping the two books apart is what makes the direction obvious: burr points at clearance and deburring, dimensions point at alignment and feed. Driving burr to zero is not the goal either: over-polish rounds the apertures within 3 mm of the edge, and an 80 μm hole swells to 88 μm with the open area following. If a customer only writes 'clean edge' on the requirement, ask for three numbers instead — 5 μm height, 15 μm root width, Ra 0.4 μm — or acceptance has nothing to stand on. Run a hand along the edge before winding; anything that catches is already out. What this basis delivers is coil with width inside ±0.05 mm, burr ≤5 μm and all five sample points passing.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292
Email:yw9@zldsmt.com
Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋