Electroformed code disc deposit thickness uniformity asks how tightly the spread is held across a single disc, which is a different question from thickness binning: binning sorts disc against disc, while this is about the disc being even with itself. It is measured on an XRF gauge against a fixed sampling map, one point at centre plus eight points each on the 0.5R and 0.9R rings, 24 points in total, giving range and non-uniformity. The nickel-cobalt deposit is nominally 30 μm, within-disc range held to 3 μm and non-uniformity ≤10%. Thickness rising and falling around the circumference makes the aperture edge's light flux wobble with it, and output signal amplitude scatters, which the scope shows immediately.
Within-disc thickness variation announces itself on the line in three ways. The first is scattered signal amplitude: discs from one batch read 3.8 V and 3.3 V on channel A, no threshold passes all of them, and the assembled unit throws angle codes. The second is within-disc deviation misread as a material issue: incoming inspection measures only the centre at 30 μm and releases, then the 0.9R ring turns out to sit at 25 μm once assembled and the edge tracks wear through early. The third is mixed measurement methods, one person subtracting substrate thickness on a micrometer, another tapping the centre alone on XRF, and the two data sets will not go on one chart. All of it points to one gap in electroformed code disc deposit thickness uniformity: no sampling map, no range criterion, no linked test procedure.
Parameter Window
• Nominal thickness 30 μm, within-disc range over the 24 points ≤3 μm, single point allowed ±2 μm from nominal.
• Sampling map fixed: 8 points each on 0.5R and 0.9R rings plus one at centre, XRF spot φ1 mm.
• Current density 1–4 A/dm², with the 0.9R outer band 0.5 A/dm² below centre to hold the thick edge down.
• Bath temperature 45±2 °C, pH 3.8–4.2, logged every shift; a swing past 0.2 goes on the thickness curve as a note.
• Linked amplitude check: full-revolution scan of 3600 tracks, amplitude range ≤0.3 V, anything worse traced back through the thickness map.
• After the 120–150 °C anneal for 2 h, thickness is re-measured and shrinkage ≤0.2 μm before release.
Manufacturing Process (8 Steps)
1. Substrate levelling — stainless disc face trued to 0.05 mm flatness, clamped without adding stress.
2. Coating and exposure — LDI at 8 μm/8 μm resolution, tracks 50 μm±0.5 μm, double-sided alignment ±5 μm.
3. Development — image measurer checks for notches afterwards, edge features biased 0.5 μm on the artwork.
4. Electrodeposition — current density staged across 1–4 A/dm², outer band 0.5 A/dm² lower to slow growth.
5. Stripping — the disc lifts from a substrate corner at a shallow angle; prying distorts the thin edge.
6. Anneal and levelling — 2 h at 120–150 °C releases stress, one rolling pass, then thickness is measured.
7. Thickness re-measurement — the 24-point map yields range and non-uniformity; discs past 3 μm go back for added deposit or are scrapped.
8. Linked amplitude scan — full-revolution scan on the flux bench, amplitude chart archived against the thickness map.
Core Advantages
1. The 24-point map puts within-disc deviation on the table, so electroformed code disc deposit thickness uniformity can finally be discussed apart from thickness binning.
2. Dropping the outer band 0.5 A/dm² holds the thick edge, and the 0.9R ring no longer runs 4 μm above centre.
3. Overlaying the thickness map on signal amplitude shows those 3.3 V discs are mostly thin-edge discs, and rework direction is set at once.
4. Bath temperature and pH logged every shift let thickness drift be traced back to the bath instead of blamed on equipment.
5. A 3 μm range criterion is a number; inspectors judge against it rather than arguing over whether uniformity is good.
6. XRF and cross-section methods are compared each quarter, and both instruments stay in use only while they agree within 0.3 μm.
Typical Applications
1. Metal code discs for incremental encoders, where A/B amplitude consistency rides directly on thickness distribution.
2. Multi-ring absolute discs, where ring-to-ring thickness error makes the inner rings lose signal first.
3. Rotary and linear gratings, where aperture edge thickness sets moiré fringe contrast.
4. Thin 0.10–0.15 mm discs for high-speed servos, where a heavy edge upsets balance.
5. Encoder final calibration lines, where discs with amplitude range past 0.3 V stop at end test.
6. Export orders requiring RoHS papers and the 24-point thickness map with the disc.
Design and Selection Notes
1. Set the within-disc range before the nominal thickness; putting electroformed code disc deposit thickness uniformity at 3 μm on the drawing is far more checkable than the words uniform deposit.
2. Tighter uniformity is not automatically better. Pushing range under 1 μm needs auxiliary anodes and doubles the cost.
3. If the 0.9R ring runs more than 2 μm above 0.5R on two lots running, go back to bath circulation and baffle position.
4. XRF spot size belongs on the inspection card; readings from φ1 mm and φ3 mm spots do not mix.
5. Thin and thick discs get separate current-staging tables; one parameter set cannot serve both thicknesses.
6. Keep amplitude and thickness re-measurement at one station instead of finding thin edges at final assembly.
7. Run the 24-point map at prototype stage; sampling 8 points in production leaves the edge rings unchecked.
Electroformed code disc deposit thickness uniformity comes down to one figure, the within-disc range: 3 μm inside is acceptable, past 5 μm there is no point hoping for steady signal amplitude. The inspector walks the 24-point map on XRF, fills range and non-uniformity into the report, then scans full-revolution amplitude on the flux bench. Overlay the two charts and thick-edge and thin-edge discs separate on the spot, so the call between extra deposit and scrap does not wait until tomorrow. Within-disc thickness deviation and thickness binning go into the contract as two items: one governs how even this disc is, the other governs sorting across the lot. For orders with hard code disc signal amplitude re-measurement requirements, freeze the sampling map, the spot size and the range line together, run production against that card, and the arguments mostly disappear.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292
Email:yw9@zldsmt.com
Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋