An electroformed part drawing review lines the customer drawing up against the process window before any material goes into the bath: thickness between 15–200μm, minimum aperture ≥25μm, hole position ±7μm and the part goes straight to scheduling; a dimension sitting on the edge gets a redraw talk; one that cannot be grown gets a straight refusal. It is not a judgement on how elegant the design looks. It is whether this drawing can come out of a nickel bath at all. Three verdicts exist: accept, accept after redraw, and cannot be made, and each one goes on paper.
Three rejections show up again and again on the floor. A stencil drawing calling 20μm apertures comes out of development with a bell-shaped mouth and the vision system reads it 4μm small. A screen with 40μm between holes lets nickel bridge sideways until two holes become one slot. Then a whole aperture plate toleranced at ±2μm, scanned on the automatic inspection machine, lands at Cpk 0.9. None of these is a craft problem. The drawing missed the window, and the review should have caught it before the quotation went out. A review that only traces the outline will meet all three at first-article stage.
Parameter Window
• Thickness 15–200μm is accepted directly; below 15μm, hole wall ≤0.01μm and tension 10–55N are hard to hold at the same time.
• Minimum aperture ≥25μm, pitch ≥120μm and hole spacing ≥50μm: all three at the limit means the development margin gets rechecked.
• Hole position ±7μm and aperture ±3μm are routine; a ±2μm call adds LDI double-side registration ±5μm plus full inspection.
• Lot size 1–500 pieces: a single part is released as a sample, while 500 and above needs Cpk ≥1.33 process data.
• Measurement basis stated up front: Cpk ≥1.33 means a controlled process; at 1.0 or below we suggest a redraw or a split part rather than tighter sampling.
• Substrate up to 610×660mm; beyond that the panel is split, and hole position ±7μm either side of the seam is called out separately.
Manufacturing Process (8 Steps)
1. Drawing intake — check format, revision and units; where DXF and PDF disagree the dimension text wins, and one question goes back before anything moves.
2. Read the critical dimensions — circle aperture, pitch, hole position, thickness and flatness, and flag which of them are functional.
3. Judge the process window — the heart of an electroformed part drawing review: compare line by line, mark anything within 10% of a limit in yellow, and log it as a cost and risk item.
4. Fix substrate and mask route — stainless mandrel or nickel plate, dry film or laminated LDI, chosen against 8μm/8μm resolution.
5. Slot scheduling — arrange by tank run and witness-panel position; a rush insert pushes the re-measurement window of that same run aside.
6. Inspection plan — decide between vision system, flash measurer and automatic inspection machine, and write sampling ratio and decision owner into the order.
7. Quotation — weight thickness, precision, lot size and re-measurement, priced against the drawing, with no off-the-cuff range.
8. Sign-back — compress redraw advice, acceptable scope and acceptance basis into a one-page sheet, signed by both sides before material is issued.
Core Advantages
1. A part inside all three limits gets its verdict the same day, without waiting for a scheduling meeting.
2. Borderline sizes are not refused on sight; we first calculate whether relaxing 1–2μm still protects the function, then propose that size.
3. For a 20μm aperture we say why it cannot be held, then offer 25μm or a two-piece split.
4. Full panels above 400 holes per square centimetre are split and stitched, with the seam routed away from functional areas and pads.
5. A refusal carries a reason: 8μm thickness at ±2μm is not physically reachable, so we decline instead of stalling.
6. Deviation is graded, not negotiated: aperture off by ±3μm where paste volume suffers goes to rework, hole position off by ±7μm is scrapped.
Typical Applications
• Precision stencil — 15–200μm thickness with ≥25μm apertures; pitch 120μm is the line between feasible and not.
• Step stencil — step location and ±3μm on each zone, plus which face contacts the board, decide the transition width.
• Electroformed screen — true roundness ±0.002mm and hole spacing ≥50μm carry the whole screening accuracy.
• Code disc and code track — a 50μm±0.5μm track width; burrs past 2μm make the read go soft.
• Aperture plate — 20μm rib width, with rib root radius and rib pitch both dimensioned, otherwise nothing can be judged.
• Ball-placement and probe template — overall pitch ±7μm and minimum aperture 30μm, supplied together with lot size and re-measurement needs.
Design and Selection Notes
1. File format: DXF or STEP plus a dimensioned PDF, revision number in the file name, never a folder called final.
2. List critical dimensions in their own table, functional holes separate from the rest, so an electroformed part drawing review does not have to guess.
3. State whether the tolerance is per piece or per lot, and give the sampling ratio that goes with ±3μm.
4. Volume and rhythm: how many for the first run, how many per month after, and how often a rush order lands, all of which shape witness-panel planning.
5. Inspection standard: which machine, sampling or full inspection, and who signs off, written into the technical requirements.
6. Delivery form: loose part, AB adhesive frame, or tensioned assembly, with packing and cleanliness class spelled out.
7. Special requirements ticked one by one: RoHS, non-magnetic, annealed condition, hardness HV450–550. Verbal mentions get lost.
An electroformed part drawing review is not fault-finding; it moves rework cost one step earlier. Whether a drawing can be made usually has an answer within two hours of receiving it, and the hard part is explaining the near miss. The yellow lines on the review sheet are mostly where rework and argument begin later. Talking the window through openly costs far less than accepting the order and explaining afterwards. If hole tolerance tightens from ±7μm to ±5μm, we go back to development and registration for two re-measurements and answer with data, not with stricter sampling.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292
Email:yw9@zldsmt.com
Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋