A metal mask plate is a pierced nickel foil made by electroforming nickel into a photoresist pattern and lifting the whole sheet off the substrate. The edge burr is the ring of protrusion or resist residue where an opening wall meets the top face. Zhuhai electroformed mask processing serves customers in Zhuhai and the surrounding area with a delivery and communication baseline that accepts burr alongside opening line width and flatness. On the floor an optical comparator reads the edge profile at 200x and burr height is judged against ≤3 μm. An out-of-spec sheet is locally dressed first and scrapped if dressing fails. Nobody signs it off on a visual no-burr claim.
Three failure modes show up on the line, each with its own source. Development can leave a thin film of resist at the base of a wall; nickel grows sideways along it and a lip appears under the opening after release, eating a micrometre or two out of a 20 μm rib. Push current density past 4 A/dm² and the corners grow fast with coarse grain, building nickel nodules at the mouth that are invisible to the eye yet block evaporation. Let developer temperature drift two or three degrees out of the 23±2 ℃ window and stress spreads unevenly, so thin walls wrinkle while the opening edge curls. A flash measurement scan tells the inspector at once that these faults do not originate at exposure; the cause sits in an earlier parameter.
Parameter Window
• LDI resolution 8 μm/8 μm, double-side alignment ±5 μm; the opening artwork is fixed here
• Aperture rib/line width 20 μm, tolerance ±0.5 μm; burr directly consumes usable line width
• Edge burr height ≤3 μm, read from the profile on a comparator at 200x
• Wall roughness ≤0.01 μm; burr and wall finish respond to the same current density
• Current density 1–4 A/dm²; above 4 A/dm² the corners tend to build nodules
• Substrate up to 610×660 mm, with zoned temperature control across a shared bath and developer held at 23±2 ℃
Manufacturing Process (8 Steps)
1. Drawing review — mark line width, burr limit and inspection face on drawings commonly received from customers in Zhuhai and nearby areas.
2. Substrate cleaning — degrease and deoxidise before conductivising; any residue left behind becomes a burr seed.
3. Resist coating and LDI — expose at 8 μm/8 μm resolution with ±5 μm double-side alignment.
4. Development — flush resist residue from wall bases and hold developer temperature at 23±2 ℃.
5. Electroforming — step the current density through 1–4 A/dm² and drop the edge zones by one band.
6. Release — after a low-temperature anneal lift from the low-stress edge, avoiding a hard pull that drags out an edge lip.
7. Inspection — comparator measures line width and burr height, flash tester scans wall roughness down to ≤0.01 μm.
8. Re-measure and pack — archive every sheet against the inspection report, shipping measured values rather than a grade promise.
Core Advantages
1. Burr is quantifiable — edge protrusion is logged as ≤3 μm in the report, never released on visual judgement.
2. Line width holds shape — the 20 μm rib is measured before and after dressing so the micrometres lost are written down.
3. Two-side register — ±5 μm alignment keeps front and back opening edges in line and reduces evaporation ghosting.
4. Large-panel bath — multiple sheets up to 610×660 mm share one bath, with zoned temperature control suppressing edge spread.
5. Rework has a basis — an over-burr sheet is dressed locally first, scrapped if that fails, and the record feeds back to development and current.
6. Open delivery — every sheet from zhuhai electroformed mask processing carries a report with line width and burr as measured figures.
Typical Applications
• Evaporation masks, where edge burr directly blurs the boundary of the deposited layer.
• Aperture plates, where a 20 μm rib and a ≤3 μm burr together set the clear cross-section.
• Semiconductor pattern-transfer masks accepted at 8 μm/8 μm resolution and ±5 μm alignment.
• Large panel masks up to 610×660 mm, relying on zoned temperature control to level edge differences.
• Through structures whose opening edges on both faces must pass comparator re-measurement.
• Prototype lots for optoelectronic customers in Zhuhai and nearby areas, judged sheet by sheet against the burr limit on the drawing.
Design and Selection Notes
1. Put the burr limit on the drawing first. A request that only says remove burr leaves acceptance to an argument about appearance.
2. Do not skimp on the development rinse. A film left at the wall base becomes a ring of edge burr after plating.
3. Current density is not the higher the better. Past 4 A/dm² the corner nodules are harder to repair than a burr.
4. If temperature drifts more than 2 ℃, go back to the development and plating stations and re-measure line width and wall.
5. Match a 20 μm rib to a ±0.5 μm tolerance and pick dressing media that respects that allowance.
6. The 200x comparator sets the reading basis; a different instrument needs a comparison on the same sample first.
7. Log burr, line width and flatness separately instead of collapsing them into one vague accuracy grade.
Focusing zhuhai electroformed mask processing on opening edge burr is not a new way of talking about mask accuracy; it moves acceptance onto the item that can actually be measured. Burr enters from development residue, from current overshoot and from the release method in turn, and the ≤3 μm reading at 200x gives every sheet a number that can be checked again. Drawings from customers in Zhuhai and nearby areas translate into stations on the process card: 8 μm/8 μm resolution, ±5 μm alignment, a 20 μm rib and a 1–4 A/dm² current, with any drift traced back to its own station. Burr and line width are delivered on the inspection-report basis, given as measured bands with their boundary conditions rather than a promise of a perfectly burr-free state. What decides whether a lot is usable is whether a dozen sheets from one bath all leave with the same set of re-measurement data; that traceable line is where zhuhai electroformed mask processing earns its value.
Contact:赖先生
Phone:+86 18938693450
Tel:0755-2708-8292
Email:yw9@zldsmt.com
Add:深圳市宝安区福永镇新和村福园一路华发工业园A3栋